Skip to main content

Table 5 Results of flexural strength in A, B, and C groups (MPa, mean ± SEM)

From: Degraded and osteogenic properties of coated magnesium alloy AZ31; an experimental study

Group

2nd week

4th week

8th week

12th week

A

266.45 ± 2.57

241.88 ± 0.86

202.72 ± 3.14

148.34 ± 2.66

B

307.45 ± 1.78

281.78 ± 5.96

244.30 ± 8.00

184.28 ± 3.94

C

319.57 ± 8.85

296.25 ± 2.74

260.66 ± 2.69

217.43 ± 2.21

  1. Group A means magnesium alloy AZ31 without coating. Group B means magnesium alloy AZ31 with 10-μm coating. Group C means magnesium alloy AZ31 with 20-μm coating